Orange Peel On The Surface Of Aluminum Plate And Aluminum Coil

Jan 03, 2020

Leave a message

Also known as pull correction

After the aluminum plate and the aluminum coil are stretched and straightened, uneven wrinkles like orange peel appear on the surface, which are called orange peels or stretch marks.

Cause:

1: When the aluminum plate is stretched and straightened, the tensile straightening rate is too large, exceeding 3%;

2: Insufficient ingot homogenization or unreasonable production process results in coarse grains.

Prevention and Control Measures:

1: Strictly control the straightening rate (0.5%-3%) until the product is straightened;

2: Strictly implement the aluminum plate production process, improve the uniformity of the product, and prevent the generation of coarse grains.