1. Surface aspects:
(1) Embossing: The irregular color difference of the roll surface caused by the wrinkle of the strip, the broken strip and other reasons during the rolling process periodically printed on the strip surface.
(2) Abrasions: appear as bundle-shaped scars on the surface of the aluminum plate. Cause: The aluminum plate is caused to shift between layers mechanically or manually.
(3) Edge warping: After rolling or shearing, the edge of the strip is warped.
(4) Corrosion: white or black spots on the surface of the aluminum plate. Cause: Acid, alkali or water has entered during production, packaging, transportation and storage.
(5) Oil on the surface: the surface is dirty. Cause: The cooling oil is dirty, and the blowing is weak.
(6) Scratches: It appears as scratches on the surface of the aluminum plate. Causes: The guide plate or flat roll has protrusions or sticky aluminum; scratches occur during cutting; manual inspection is not carried properly.
(7) Side edge bending: The longitudinal sides of the plates and strips are in a non-straight state bent to one side. Causes: The rolling reductions at the two ends of the rolling mill are not the same; the thicknesses of the two sides of the plate and the belt are not consistent.
(8) Black spots on the surface: There are needle-like black spots on the surface of the aluminum plate. Cause: The furnace fluid is not clean.
2. In terms of mechanical properties:
(1) The hardness is insufficient. Reason, material / composition, heat treatment process.
(2) Cracking on stamping, hard or soft. Material or condition issues.
(3) Other defects: water ripples, black and white channels after oxidation; dark surface on the surface.